The durability characteristics and microscopic mechanism of cement-based silica
dust foam lightweight soil were investigated by using cement and silica dust as
cementitious materials to create foam lightweight soil. The unconfined
compressive strength, apparent morphology, mass loss rate, and pore structure
were determined by analyzing the wet density (500, 600, 700, and 800
kg/m^3), silica dust content (0%, 7.5%, 12.5%, 17.5%, 22.5%), and
the number of cycles of freezing and thawing. The results show that when the
number of freeze-thaw cycles rises, the unconfined compressive strength shows a
shifting negative trend. The apparent morphology of specimens with wet densities
more than 700 kg/m3 was rather intact after 30 freeze-thaw cycles. Additionally,
the mass loss rate for each specimen is less than 5%. The unconfined compressive
strength may be significantly increased when the quarry’s dust concentration is
less than 12.5%. The design wet density is exactly related to the compressive
strength at the same curing age. A prediction method for the freeze-thaw cycle
performance of lightweight soil made of silica dust foam and cement with various
mix ratios was developed based on the experimental findings. The porosity of
foamed light soil decreases with increasing wet density, according to the
microscopic mechanism of freeze-thaw cycle strength. The average pore size
decreases with increasing silica dust addition. The study’s findings may serve
as a foundation for this material’s engineering use.